First make sure the crack has stopped growing, which means the slab is dry. Then pick a fix. Bow ties (also called butterfly keys) set across the crack hold it from spreading. Epoxy fills the gap and seals it. Many slabs get both: bow ties for strength and looks, epoxy to fill what's left. A crack near the end is often better cut off than fixed.
Here's how to choose, and how to do each one.
Step one: is the crack still moving?
Every fix depends on this. A bow tie or epoxy fill on a slab that's still drying can't stop the wood from shrinking. The crack opens beside the fix, or a new one starts nearby.
Check:
- Moisture readings in several places away from the ends. See how to check whether a slab is dry.
- The inside of the crack. Gray, weathered wood suggests an old crack. Bright, clean wood suggests a new one.
- The tip. Mark the end of the crack with a pencil line and check it again in a few weeks. If it's grown, wait.
Not every crack needs fixing; why slabs crack and cup sorts the harmless ones from the rest.
Your options
| Fix | Best for | Strength | Look |
|---|---|---|---|
| Bow ties | Through-cracks you want to keep | Holds the crack from spreading | Decorative, handmade |
| Epoxy fill | Gaps, voids, knot holes, checks | Seals and fills; adds little strength across a crack | Clear, tinted or black |
| Bow ties plus epoxy | Wider through-cracks | Best of both | Most common on tables |
| Thin CA glue | Hairline checks | Minimal | Nearly invisible |
| Cut it off | Cracks near the end | Removes the problem | Shorter slab |
| Rip and reglue | One straight crack down a slab | Strong glue joint | Crack disappears |
Bow ties
A bow tie is a small piece of wood shaped like a bow tie, set into a matching recess across the crack. The flared ends lock into the wood on both sides, so the crack can't open wider.
Orientation. Set each bow tie across the crack, with its narrow waist over the crack line and its long axis at right angles to it. Make the bow tie so its grain runs along that long axis, across the crack. Grain running the other way makes a weak key that can split at the waist.
Placement. Put one near the tip of the crack, slightly beyond where it ends, to stop it from running further. Add more along the crack's length as needed. Uneven spacing often looks more natural than a neat row.
Depth. Deep enough to grab solid wood on both sides. Shallow, decorative keys look the part but hold little. If the crack goes through, consider keys on the underside too.
Material. Use a hard, stable, dry wood. Contrast is common: dark keys in a pale slab, pale keys in a dark one.
How to make them:
- Make the bow ties first, from dry stock with the grain running end to end.
- Lay each one on the slab across the crack and trace around it with a sharp knife or fine pencil.
- Rout out most of the recess inside the line, using a template guide or an inlay kit if you have one, and stay just shy of the line.
- Pare the walls and corners to the line with a sharp chisel. Test the fit often. You want snug, not hammered in.
- Glue the recess walls and the key, tap it home and let the glue cure.
- Plane, rout or sand it flush with the surface.
Epoxy fills
Epoxy fills gaps, voids, knot holes and checks, and seals them so they don't collect crumbs. On its own it adds little strength across a through-crack; pair it with bow ties if the crack runs through.
Tape the back. If the crack goes through, cover it on the underside with packing tape or sheathing tape so epoxy doesn't run out. Press it down hard along the crack.
Seal the wood first. Brush a thin coat of epoxy into the crack and let it set. That reduces bubbles from air escaping the wood.
Check the product's maximum pour depth. Epoxy formulas differ a lot. Thin tabletop epoxies are made for shallow coats; deep-pour formulas are made for thicker fills. Pouring past the label's limit in one go can make it overheat, crack or yellow. For a deep crack, fill in layers and let each cure according to the label.
Tint if you want. Black or dark epoxy hides the crack's outline and reads like a natural line. Clear lets you see into the crack. Colored epoxy makes a statement.
Overfill slightly. Epoxy settles as it soaks in and cures. Leave it a little proud of the surface.
Pop bubbles. A quick pass of a heat gun or torch over the surface releases bubbles. Keep it moving and don't overheat the wood or the epoxy.
Level it. Once fully cured, plane, rout or sand it flush. If you're flattening the slab anyway, fill before the final flattening pass so one pass levels both.
Thin CA glue for hairline checks
For small surface checks that don't go through, thin cyanoacrylate (CA) glue wicks into the crack and hardens. Sand it flush after. It's quick, nearly invisible, and keeps the check from catching finish or dirt.
Cut it off
A crack that runs in from the end is often a cut-off, not a fix. Mark the tip of the crack, add a little extra, and trim the slab square there. If you need the length, stabilize it; if you don't, the cleanest repair is a saw.
That's one reason to buy a slab longer than your finished piece.
Rip and reglue
If a slab has one straight crack down its length, you can rip it along the crack, joint both edges straight and glue the two halves back together. The crack disappears into a glue line. You lose the width of the saw cut and the natural crack, and the grain at the joint may not match perfectly.
What about cracks you can't see?
Sometimes flattening opens up a crack that wasn't visible in the rough slab. Deal with it the same way: confirm the slab is dry, then key, fill or both. See flattening a slab with a router sled for when to fill relative to flattening.
On a river table, cracks are often filled in the same pour as the river; the river table guide covers that.
For how cracks affect what a slab costs, see our pricing page, or browse our slabs page.
Ask About a Slab
Tell us the size of the piece you need and ask how a slab's cracks would affect it: whether they go through, how far they run, and how much length is left if you cut them off.